Wetting and Spreading Behavior of Liquid Si-Ti Eutectic Alloy in Contact with Glassy Carbon and SiC at T = 1450 °C
Authors/Creators
- 1. National Research Council of Italy-Institute of Condensed Matter Chemistry and Technologies for Energy, Via De Marini 6, 16149 Genova, Italy
- 2. Foundry Research Institute, Zakopiańska 73 Str., 30-418 Krakow, Poland
Description
The contact heating sessile drop and capillary purification methods were applied for a fundamental study concerning the wettability and reactivity of liquid Si-16.2at%Ti (eutectic composition) in contact with Glassy Carbon and SiC at T = 1450°C under an Ar atmosphere. Different spreading stages with different slopes, depending on the starting conditions of the materials used, where observed. On the contrary, the final contact angle value seemed not affected and the equilibrium contact values of θ ≈ 44°± 2 and θ ≈ 42°± 2 where displayed on Glassy Carbon and SiC, respectively.
The solidified Si-Ti eutectics/GC and Si-Ti eutectics/SiC samples were examined both at the top of
the drop and at the cross-section by SEM/EDS. The presence of a SiC layer as unique reaction product at the Si-Ti eutectics/GC interface, confirmed that wettability is mainly driven reactivity.
Contrarily, as non-reactive system, at the Si-Ti eutectics/SiC interface a weak dissolution of SiC substrate was detected.