Nano-sized BaSnO3 powder via a precursor route. Comparative study of sintering behaviour and mechanism of fine and coarse-grained powders.
Authors/Creators
Description
Preparation of a very fine BaSnO3 powder by calcination of a barium tin 1,2-
ethanediolato complex precursor and its sintering behaviour are described herein. A rate
controlled calcination process to 820 °C leads to a nm-sized BaSnO3 powder with a
specific surface area of S = 15.1 m2/g (dav. = 55 nm). The powder has a slightly larger
cell parameter of a = 412.22(7) pm compared to the single crystal value, which
decreases with increasing calcination temperature and reaches the reference value above
1000 °C. The sintering behaviour is compared between fine- and coarse-grained
BaSnO3 powders. Corresponding powder compacts of the nano-sized BaSnO3 achieve a
relative density of 90 % after sintering at 1600 °C for 1 h and at 1500 °C and a soaking
time of 30 h, whereas coarse-grained powder compacts reach only 80 % of the relative density at 1650 °C (10 h). Furthermore, the shrinkage mechanisms of fine and coarsegrained powder compacts have been investigated and are discussed.